» Process for Color Anodizing

DEGREASING :- Removal of oil, grease & oxide coating from aluminium surface.


PRODUCT

NATURE

CONC.

TIME

TEMP.

ALKLIN HD

Alkaline Degreasing

5% w/v

5-15 min

RT to 65°C

ETCHING :- Chemical finishing of degreased aluminium surface.


PRODUCT

NATURE

CONC.

TIME

TEMP.

ALCLEANSER

Acidic Etching

3-5% v/v

10-15 min

RT

DESMUTING :-  To remove traces of black smut left .


PRODUCT

NATURE

CONC.

TIME

TEMP.

NITRIC ACID

-

5% v/v

2-5 min

RT

ANODIZING :- Electrochemical Conversion process leaving porous oxide coating on aluminium surface.


PRODUCT

CONC.

TIME

VOLTAGE

CURRENT DENSITY

TEMP.

SULFURIC ACID

180-200 gm/lit

30 min

14 to 18 V D.C.

10 – 15 A / Sq. Ft.

15 -20°C

COLORING :-
Electrolytic Coloring – Electro deposition of metallic color particles into the anodic coating.


PRODUCT

NATURE

CONC.

TIME

VOLTAGE

TEMP.

ALCOL - P

Metallic salt.

10-15 gm/lit

15 sec to 15 min depending upon the colour shade required.

14 to 18 V A.C.

18 -25 °C

ALCOL ST

Colour stabilizer & throwing power improver

18 gm/lit

ALCOL L201

Liquid with combined colour and stabilizer. Easy to use.

6%  v/v

SULFURIC ACID

-

18-20 gm/lit

SEALING  :- Seals the pores of anodic coating.


PRODUCT

NATURE

CONC.

TIME

TEMP.

ALSIL  71

Impregnating metallic salts

5 gm/lit

0.5-1min/micron of anodic coating

25 to 30° C